Salt-gradient one-step heparin coating keeps 73% of heparin after 16 days in lab tests on polylactic acid

Researchers deposited a PEI–heparin anticoagulant coating in one immersion-withdrawal step. In vitro and ex vivo, it cut platelet adhesion by 98% and thrombus formation by 90%.

Salt-gradient one-step heparin coating keeps 73% of heparin after 16 days in lab tests on polylactic acid
Photo: Edward Roberts (edward.beardsell)/www.clinicccompare.co.uk, Wikimedia Commons, CC BY 2.0 · License: CC BY 2.0

Researchers have reported a one-step method for applying anticoagulant coatings to blood-contacting materials, according to a paper in Surface Science and Technology. The coating is built from polyethyleneimine (PEI) and heparin and is driven by a salt-concentration gradient. The tests were laboratory and ex vivo experiments on polylactic acid substrates; the coating has not been reported in clinical use. springer.comSurface Science and Technologyspringer.comOpen source ↗

Surface-induced thrombosis limits the safety of blood-contacting devices. Surface heparinization is widely used to improve hemocompatibility, but existing methods, such as covalent grafting and Layer-by-Layer assembly, are complex or not stable enough, the authors state.

How the coating is formed

The team used 4 mol/L NaCl to screen the electrostatic interactions between PEI and heparin, which gave a homogeneous precursor slurry. According to the publisher's account, the polyelectrolyte complexes were first precipitated at acidic pH, centrifuged at 5,000 rpm for 5 minutes and then redissolved in the salt solution.

Polylactic acid specimens were pretreated with dopamine, then with a dopamine and low-molecular-weight PEI solution. A tube was filled with deionized water above a layer of the high-salt slurry, forming a liquid interface. The substrate was immersed in the slurry and withdrawn upward through the interface into the water. springer.comSurface Science and Technologyspringer.comOpen source ↗

Salt diffuses rapidly into the water at the interface, the charge screening disappears, and liquid–liquid phase separation deposits a dense coacervate of PEI and heparin on the surface. The authors attribute the stability of the coating to physical entanglement of the polymer chains.

Withdrawal speed affected the morphology. At 5 and 10 mm/s the coating did not form a continuous film and instead formed isolated island-like clusters. At 1 mm/s the film was continuous and uniform.

Measured properties

The coated surface retained 73% of its heparin after 16 days of physiological incubation. The hemolysis rate was 0.32%, platelet adhesion was suppressed by 98%, and ex vivo thrombus formation was reduced by 90%. springer.comSurface Science and Technologyspringer.comOpen source ↗

The water contact angle fell from about 83.98° on bare polylactic acid to 24.92° on the coated surface. Infrared spectroscopy showed a peak near 937 cm⁻¹ assigned to sulfate ester bonds characteristic of heparin. X-ray photoelectron spectroscopy found nitrogen (14.02 atomic %) and sulfur (2.04 atomic %) on the coating, which were absent on the bare substrate.

The authors describe the approach as a scalable assembly route for functionalizing cardiovascular implants.

Sources · 2

Found a mistake?
  1. ↩
RealTech on TelegramSubscribe

Read also

Up next

The next story opens automatically

More
Follow us

Type at least two letters — results appear instantly

↑↓to choose↵to openescto close