**Two hundred lightweight blocks in a Cambridge plantroom wall were surveyed after six years; the self-healing additives showed no detectable adverse effect on the host concrete.**

![Cambridge low-carbon and self-healing concrete blocks assessed after six years in a Dyson Building wall](https://realtech.media/media/2026/11/d01b71bf2cbce30b.jpg)
*Sadopaul, Wikimedia Commons, CC BY-SA 4.0*

Researchers at the University of Cambridge have reported six-year in-service results for low-carbon and self-healing lightweight concrete blocks in the journal Case Studies in Construction Materials. Two hundred full-size blocks (400 mm × 215 mm × 100 mm; 100 per family) were hand-manufactured in the university laboratory. With the contractor Morgan Sindall, they were installed in a non-structural internal plantroom wall of the James Dyson Building [1]. The paper reports 30 mixes: 23 low-carbon and 7 self-healing [1].

## Binders, additives and test methods

The low-carbon binders were PC–GGBS–MgO blends and slag-rich binders activated with reactive MgO, lime and/or sodium carbonate [1]. The self-healing mixes used sodium silicate microcapsules, expansive minerals or PVA-coated MgO pellets. All mixes contained Lytag lightweight aggregate [1].

Cube strengths were measured at 7 and 28 days and, for selected mixes, at 240 days. After six years the installed blocks were surveyed with a rebound hammer, ultrasonic pulse velocity (UPV), surface resistivity and Torrent air permeability. The results were interpreted as relative indices against the control of each family [1].

## Six-year results and embodied carbon

The rebound indices of the alkali-activated mixes fell within a narrow band of 0.58–0.73 × that of the PC control. Those of all self-healing mixes were within about 10% of their control [1]. Most mixes gave UPV values within the scatter of their controls [1].

PC-free slag mixes activated only by MgO and/or lime showed markedly higher air permeability, which the authors attribute mainly to weak slag activation [1]. The self-healing mixes gave UPV, resistivity and air-permeability indices similar to those of their control. According to the authors, this indicates no detectable adverse effect of the healing additives on the host concrete in this sheltered exposure [1].

The binder embodied carbon of the slag-rich and clinker-free mixes was 45–85 kgCO₂e/m³, which is 69–83% below that of the PC control. At block level, with the Lytag aggregate included, the reduction was 36–44% [1]. The authors also discuss the challenges of scale-up and of interpreting non-destructive test data for lightweight concrete blocks [1].

## Sources

1. [Case Studies in Construction Materials](https://doi.org/10.1016/j.cscm.2026.e06743)
2. [bioengineer.org](https://bioengineer.org/low-carbon-and-self-healing-concrete-blocks-demonstrate-durability-across-six-in-service-years)

---

Source: RealTech, realtech.media — https://realtech.media/news/rt-7f1d0fdb74517ba0ed790bb8_cambridge_low_carbon/